Typical Poisson's Ratios of Polymers
at Room Temperature
Polymer |
Value |
Polyacetal, Poly(methylene
oxide), POM |
0.44 |
Poly(alpha-methylstyrene),
PAMS |
0.32 |
Poly(Bisphenol A carbonate),
PC |
0.41 |
Polybutylene, PB-1 |
0.48 |
Poly(1,4-butylene terephthalate),
PBT |
0.42 |
Polycaprolactam, Nylon 6 |
0.42 |
Poly(2,6-dimethyl-p-phenylene
oxide), PPO |
0.41 |
Polyetheretherketone,
PEEK |
0.39 |
Polyethersulfone,
PES |
0.42 |
Polyethylene, HDPE |
0.46 |
Poly(ethylene terephthalate),
PET |
0.43 |
Poly(hexamethylene adipamide), Nylon 6,6 |
0.42 |
Polyisoprene,
IR |
0.50 |
Poly(methyl methacrylate),
PMMA |
0.36 |
Poly(2-methylstyrene ) |
0.35 |
Poly(4-methylstyrene),
PPMS |
0.34 |
Poly(1,4-phenyl ether),
PPE |
0.41 |
Polyphenylsulfone,
PPSF |
0.43 |
Polypropylene,
PP |
0.43 |
Polytetrafluoroethylene, PTFE |
0.42 |
Poly(p-tertiary-butylstyrene) |
0.33 |
Polystyrene,
PS |
0.35 |
Polysulfone,
PSU |
0.37 |
Poly(vinyl chloride),
PVC |
0.40 |